Total payment:
-
T12
30
Burnt-on sand
This flaw can arise in any casting produced by a sand molding method, regardless of the material employed. This defect has also occurred ...
T12
30
This flaw can arise in any casting produced by a sand molding method, regardless of the material employed. This defect has also occurred ...
T12
22
As a result of physical/chemical interactions between melt and molding material components, this fault may arise with all molds manufactu...
T12
16
What is lost foam casting? Lost foam casting is a method of producing intricate metal components and parts in which molten metal evaporat...
T12
14
Characteristics Cold crack: It is also a straight or curved crack on the casting's surface with little oxidation on the crack's sur...
T12
13
Causes of slag inclusion: - After treating the liquid iron with magnesium and rare earth, a series of reactions between the sulfur, oxyge...
T12
12
Cold shuts are more common on level surfaces with rather thick walls. As a result, cohesive material may separate, leaving holes, blank a...